sample57Žabjak Ptuj · Styria

46.433358 15.894477

Collected by Ljubica Zgonec Zorko

Pottery Wheel Throwing Demonstration – Žabjak Ptuj · Styria
Pottery Wheel Throwing Demonstration
Photo Ljubica Zgonec Zorko

Žabjak

The activity of the Centre for Handicraft and Art Craft, Rokodelska zadruga (Handicraft co-operative), is based on the preservation of cultural heritage, the transfer of traditional handicraft skills and traditions to the younger generations as well as the development and promotion of modern products. We see our mission in developing artistic creativity and education, and ensuring active spending of free time and enriching the quality of life of all generations, so we organize various exhibitions and events as well as workshops and courses on clay creation for children and adults.

Ljubica Zgonec Zorko

Sample 57 is clay from Žabjak Ptuj (Styria). The recommended firing temperature is 900–1100 °C. The beginning of sintering is at 1100–1250 °C. At 1100 °C shrinkage is 10 % and porosity 6 %.

Clay samples

  1. Sample 57 – 800 °C800 °C
  2. Sample 57 – 900 °C900 °C
  3. Sample 57 – 1000 °C1000 °C
  4. Sample 57 – 1100 °C1100 °C
  5. Sample 57 – 1200 °C1200 °C
  6. Sample 57 – 1300 °C1300 °C
segrevanjeheating uppriporočena temp. žganjarecommended firing temperatureszačetek sintranjathe beginning of sinteringmehčanjesofteningžganje/firing °C%%00224466881010121214141616181820202222suha glina/dry clay900 °C1000 °C1100 °C1200 °C1300 °C
  • segrevanje
    heating up
  • začetek sintranja
    the beginning of sintering
  • mehčanje
    softening
%048121620suhadry9001000110012001300°C
poroznost/porosity %skrčki/shrinkage %

Clay preparation for testing

  1. unprocessed clayunprocessed clay
  2. sifted and dried claysifted and dried clay
  3. 012341.00.20.05%grain size in mm
  4. 1.5 % = 1.0 mm1.5 % = 1.0 mm
  5. 0.5 % = 0.2 mm0.5 % = 0.2 mm
  6. 0.5 % = 0.05 mm0.5 % = 0.05 mm